Composition and test results for Taurina stone and for carparo / tufa, extracted from open-pit quarries in Salento.
Marly calcarenite of the Miocene
A granular mix of microfossils, fossil fragments, intraclasts and pellets held together by calcitic cement. Calcium carbonate makes up 93–95%.
Small amounts of glauconite, quartz, feldspars, muscovite, phosphates and clay materials affect colour and hardness. Because of the Miocene lithofacies of Salento, the stone comes in several types that differ in colour, grain size, homogeneity, compactness and age.
After 20 freeze-thaw cycles, the tested sample showed no cracks or signs of damage, and the loss of compressive strength was below 20%.
| Bulk density | 1,686 kg/m³ |
| Specific weight | 2,577 kg/m³ |
| Water absorption | 15% |
| Porosity | 35% |
| Compressive strength, dry | 179 kg/cm² |
| Compressive strength, wet | 134 kg/cm² |
| After frost test | 130 kg/cm² |
| Flexural strength, dry | 34.6 kg/cm² |
| Modulus of elasticity | 14,550 kg/cm² |
| Sand-blast wear | 2.7 g |
| Impact resistance | 0.94 kgm |
Warm, rustic and well tested
Average chemical composition: calcium carbonate 97.51%, magnesium carbonate 1.38%, silica 0.54%, ferric oxide 0.14%, organic carbon 0.11%.
Compressive strength (cubes 7.2 cm): 41.4–73.4 kg/cm² natural, 42.8–82.9 kg/cm² saturated, 35.0–58.0 kg/cm² after the frost test.
| Specific weight | 2.72 g/cm³ |
| Dry bulk density | 1.58 g/cm³ |
| Saturated bulk density | 1.87 g/cm³ |
| Compactness index | 0.51 |
| Flexural strength, natural | 19.2–27.5 kg/cm² |
| Flexural strength, saturated | 10.9–21.0 kg/cm² |
| Flexural strength, frost-tested | 9.42–15.3 kg/cm² |